Magnesium Mg95, R0 =  1.738 g/cc

Target: Magnesium Mg95, "original" cast magnesium
  Sample density R0 = 1.738 g/cc, bulk sound velocity C0 = 4.5 km/s, longitudial sound velocity Cl = 5.61 km/s
  Sample thickness 9.93 mm (bar)
  Initial temperature 585 C
Loading: 
  Aluminum impactor 1.99 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.052      0.690
      0.084     14.500
      0.102     31.300
      0.114     51.146
      0.122     71.700
      0.125     89.242
      0.159     95.300
      0.202    112.100
      0.212    135.700
      0.226    152.500
      0.266    176.100
      0.302    192.900
      0.315    216.500
      0.324    233.300
      0.394    763.316
      0.413    798.900
      0.459    822.500
      0.509    827.680
      0.626    821.869
      0.720    801.411
      0.786    782.100
      0.842    763.316
      0.887    741.700
      0.948    718.100
      0.971    707.937
      1.009    692.060
      1.016    701.300
      1.041    718.100
      1.076    746.032
      1.134    772.134
      1.187    782.100
      1.246    787.120
      1.316    782.100
      1.454    766.640
      1.563    774.840
      1.737    773.100

References:
1. G. I. Kanel\', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)