Magnesium Mg95, R0 =  1.738 g/cc

Target: Magnesium Mg95, "original" cast magnesium
  Sample density R0 = 1.738 g/cc, bulk sound velocity C0 = 4.5 km/s, longitudial sound velocity Cl = 5.61 km/s
  Sample thickness 10.02 mm (bar)
  Initial temperature 600 C
Loading: 
  Aluminum impactor 1.95 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.027     23.820
      0.079     67.280
      0.117     42.570
      0.164     62.787
      0.198    105.320
      0.219    131.900
      0.236    188.360
      0.244    214.815
      0.254    349.820
      0.266    457.900
      0.271    539.400
      0.277    594.320
      0.295    690.300
      0.316    757.320
      0.336    783.900
      0.361    801.411
      0.401    812.290
      0.463    807.055
      0.557    786.596
      0.636    757.320
      0.758    691.680
      0.827    754.497
      0.878    772.134
      0.966    766.138
      1.170    744.320
      1.408    752.610
      1.841    752.490
      2.491    748.480

References:
1. G. I. Kanel\', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)