Magnesium Mg95, R0 =  1.738 g/cc

Target: Magnesium Mg95, "original" cast magnesium
  Sample density R0 = 1.738 g/cc, bulk sound velocity C0 = 4.5 km/s, longitudial sound velocity Cl = 5.61 km/s
  Sample thickness 1.93 mm (bar)
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.088      1.060
      0.101      1.500
      0.120      2.000
      0.126     34.160
      0.158     74.560
      0.174    114.960
      0.177    155.360
      0.206    783.069
      0.208    806.349
      0.223    821.164
      0.237    817.989
      0.249    812.346
      0.261    791.887
      0.272    761.360
      0.290    720.960
      0.305    686.772
      0.319    648.677
      0.334    604.938
      0.345    575.661
      0.360    539.430
      0.375    575.661
      0.386    602.116
      0.395    616.578
      0.410    624.940
      0.424    619.753
      0.442    599.760
      0.471    567.196
      0.493    543.010
      0.521    575.661
      0.542    593.000
      0.562    598.230
      0.582    593.000
      0.619    559.360
      0.638    548.000
      0.655    564.021
      0.675    585.000
      0.695    590.070
      0.709    585.000
      0.739    559.360
      0.764    553.000
      0.783    559.360
      0.821    571.310
      0.884    566.210
      0.954    570.430

References:
1. G. I. Kanel\', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)