Titanum VT6, R0 =  4.450 g/cc

Target: 
  Sample density R0 = 4.45 g/cc, bulk sound velocity C0 = 5.12 km/s, longitudial sound velocity Cl = 6.15 km/s
  Sample thickness 9.8 mm (sheet)
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 450 +/- 20 m/s
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.100    100.000
      0.140    145.000
      0.200    158.000
      0.240    169.000
      0.280    187.000
      0.300    200.000
      0.350    233.000
      0.400    275.000
      0.450    307.000
      0.500    318.000
      0.550    321.000
      0.600    318.000
      0.674    299.118
      0.796    239.577
      0.900    166.000
      1.000     93.000
      1.100     50.000
      1.200     37.000
      1.300     33.000
      1.400     30.000
      1.600     28.000
      1.900     24.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)