Titanum VT6, R0 =  4.450 g/cc

Target: 
  Sample density R0 = 4.45 g/cc, bulk sound velocity C0 = 5.12 km/s, longitudial sound velocity Cl = 6.15 km/s
  Sample thickness 18.4 mm (sheet)
Loading: 
  High explosive in contact with sample
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.100    140.000
      0.210    163.951
      0.300    189.000
      0.370    240.000
      0.473    598.236
      0.500    660.000
      0.561    691.640
      0.700    699.000
      1.000    688.000
      1.500    656.000
      2.000    619.000
      2.500    576.000
      3.000    529.000
      3.500    481.000
      4.000    430.000
      4.104    422.998
      4.200    429.000
      4.300    441.000
      4.400    460.000
      4.500    500.000
      4.700    600.000
      4.800    638.000
      4.900    650.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)