Titanum VT8, R0 =  4.450 g/cc

Target: 
  Sample density R0 = 4.45 g/cc, bulk sound velocity C0 = 5.12 km/s, longitudial sound velocity Cl = 6.15 km/s
  Sample thickness 10 mm (rod)
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 5300 +/- 150 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.040     15.000
      0.080     15.000
      0.080    350.000
      0.080    495.000
      0.080   4000.000
      0.083   4300.000
      0.089   4331.802
      0.105   4330.000
      0.170   4200.000
      0.252   3995.406
      0.270   3957.000
      0.285   4000.000
      0.310   4050.000
      0.331   4090.165
      0.350   4100.000
      0.369   4090.165
      0.439   3988.693
      0.460   3961.000
      0.470   3965.000
      0.526   4087.006
      0.540   4096.000
      0.558   4087.006
      0.617   4005.276
      0.640   3977.000
      0.657   4008.435
      0.700   4070.000
      0.720   4074.000
      0.740   4065.000
      0.830   3994.000
      0.840   3995.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)