Molybdenum, R0 = 10.206 g/cc

Target: 
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 0.75 mm (sintered rod)
  Aluminum baseplate 2 mm thick
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 660 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.023      5.390
      0.031     19.160
      0.041     95.410
      0.050    171.660
      0.066    296.000
      0.072    299.030
      0.079    297.407
      0.088    290.000
      0.100    279.000
      0.123    260.617
      0.142    244.321
      0.149    239.259
      0.160    265.802
      0.165    270.270
      0.192    260.000
      0.206    267.130
      0.234    255.000
      0.258    264.620
      0.270    260.000
      0.392    252.320

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)