Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 1.45 mm 
  Aluminum baseplate 1.45 mm thick
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 660 +/- 20 m/s
  (in direction <110>)
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.010      1.000
      0.030      2.500
      0.052      5.070
      0.058      7.000
      0.068     49.280
      0.079    100.740
      0.092     80.000
      0.095     82.000
      0.100     86.000
      0.120    130.864
      0.135    161.764
      0.142    165.340
      0.190    130.780
      0.217    108.440
      0.287     49.280
      0.322     38.140
      0.391     46.150
      0.452     36.700
      0.496     42.110

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)