Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 1.47 mm 
  Aluminum baseplate 1.96 mm thick
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 1250 +/- 70 m/s
  (in direction <110>)
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.026     10.670
      0.029     39.820
      0.037    120.000
      0.050    103.000
      0.056     97.000
      0.058     99.280
      0.063    121.320
      0.089    365.820
      0.100    423.000
      0.105    427.260
      0.150    365.820
      0.166    336.670
      0.194    284.320
      0.209    263.940
      0.217    284.320
      0.240    343.210
      0.248    348.090
      0.261    336.670
      0.299    292.580
      0.330    330.000
      0.340    334.290
      0.350    330.000
      0.391    298.420
      0.420    318.000
      0.435    326.000
      0.448    327.670
      0.460    320.000
      0.490    296.950

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)