Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 0.9 mm 
Loading: 
  High-power ion beam
  (in direction <110>)
Experiment type: Laser interferometer (ORVIS)

     t, ns      V, m/s

      0.000      0.000
      2.600    142.650
      6.800    104.280
      8.000    100.450
     11.500    124.310
     15.600    182.430
     21.000    280.650
     27.000    447.850
     30.000    485.720
     32.000    477.590
     39.000    435.340
     49.600    370.440
     58.000    318.570
     70.000    253.940
     80.457    219.224
     88.000    201.640
     89.886    220.635
     99.000    319.310
    102.000    331.220
    107.000    330.000
    113.200    322.000
    119.300    314.000
    128.500    296.670
    137.700    278.390
    147.700    268.080

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)