Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 0.416 mm 
Loading: 
  Aluminum impactor 0.05 mm thick, impactor velocity 4100 +/- 150 m/s
  (in direction <110>)
Experiment type: Laser interferometer (ORVIS)

     t, ns      V, m/s

      0.000      0.000
      1.220    124.260
      2.280     93.710
      3.000     88.000
      3.410    101.210
      4.500    183.840
      7.460    954.900
      8.050   1004.820
      8.660   1009.840
     10.340    979.340
     14.110    900.290
     18.090    796.700
     21.450    688.790
     25.100    553.620
     26.530    497.510
     28.060    666.360
     29.400    796.000
     29.890    806.580
     31.300    803.060
     35.700    750.810
     39.400    694.810
     42.700    644.040
     44.169    725.503
     45.290    740.470
     48.780    720.000
     51.900    690.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)