Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 0.286 mm 
Loading: 
  Aluminum impactor 0.05 mm thick, impactor velocity 4100 +/- 150 m/s
  (in direction <110>)
Experiment type: Laser interferometer (ORVIS)

     t, ns      V, m/s

      0.000      0.000
      1.160    135.210
      1.390    120.730
      1.500    115.000
      1.600    125.000
      2.990   1786.420
      4.580   1740.980
      6.200   1672.820
      8.100   1580.300
      9.880   1465.610
     11.900   1346.640
     13.200   1494.480
     14.000   1580.000
     14.700   1600.660
     16.690   1547.820
     20.380   1430.440
     23.240   1517.860
     25.360   1481.800
     28.600   1467.320
     31.840   1465.180

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)