Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 0.37 mm 
Loading: 
  High-power ion beam
  (in direction <110>)
Experiment type: Laser interferometer (ORVIS) (water window)

     t, ns      V, m/s

      0.000      0.000
      1.323     67.866
      1.650     91.287
      1.992    110.030
      5.873    118.120
      7.164    131.880
      8.539    167.480
      9.823    236.250
     10.621    284.390
     11.656    323.620
     13.051    354.370
     15.029    380.260
     17.355    384.300
     20.035    379.050
     22.874    363.270
     26.116    345.060
     30.000    321.200
     50.170    218.850
     53.447    206.310
     56.550    198.220
     60.361    190.130
     64.380    185.280
     67.657    185.280
     70.836    184.500
     74.238    186.890
     77.431    189.500
     80.958    192.150
     84.956    194.980
     88.608    198.220
     91.746    201.460
     95.237    207.520

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)