Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 3.88 mm 
  Aluminum baseplate 4 mm thick
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 660 +/- 20 m/s
  (in direction <100>)
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.035      4.000
      0.041      6.000
      0.050     10.000
      0.070     20.000
      0.081     40.750
      0.102    110.270
      0.140     65.000
      0.160     53.970
      0.187     57.000
      0.200     67.200
      0.260    122.250
      0.290    148.700
      0.335    203.750
      0.360    230.200
      0.397    285.250
      0.425    295.000
      0.465    299.330
      0.550    294.000
      0.616    285.250
      0.730    255.000
      0.802    223.951
      0.897    176.810
      0.990    245.000
      1.010    249.000
      1.037    250.490
      1.057    248.000
      1.225    217.470
      1.315    236.500
      1.343    238.670
      1.365    236.000
      1.503    216.640
      1.664    230.110

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)