Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 4.6 mm 
  Aluminum baseplate 5 mm thick
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 5300 +/- 150 m/s
  (in direction <100>)
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.005      2.500
      0.010      5.000
      0.014      9.000
      0.019     16.000
      0.019    395.000
      0.020   2505.000
      0.020   2768.770
      0.097   2710.480
      0.140   2655.520
      0.173   2590.780
      0.189   2649.945
      0.205   2702.362
      0.214   2711.814
      0.228   2716.850
      0.240   2709.000
      0.252   2697.000
      0.293   2670.000
      0.369   2697.090
      0.470   2696.110

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)