Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 1.4 mm 
  Aluminum baseplate 2 mm thick
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 660 +/- 20 m/s
  (in direction <100>)
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.060     11.000
      0.076     24.000
      0.087     47.750
      0.088     69.990
      0.090    136.140
      0.109    107.000
      0.115    105.000
      0.118    107.000
      0.123    129.250
      0.127    150.490
      0.139    210.750
      0.151    248.000
      0.157    250.000
      0.163    248.000
      0.195    210.265
      0.237    150.490
      0.249    129.250
      0.288     69.990
      0.310     36.000
      0.315     32.000
      0.318     29.100
      0.325     31.500
      0.364     84.000
      0.370     91.000
      0.383     93.750
      0.390     91.000
      0.400     85.000
      0.437     49.000
      0.447     45.000
      0.457     42.530
      0.467     45.000
      0.477     49.000
      0.557     70.060
      0.594     72.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)