Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 1.38 mm 
  Aluminum baseplate 2 mm thick
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 1250 +/- 50 m/s
  (in direction <100>)
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.005      4.000
      0.010      8.000
      0.028     85.430
      0.041     62.000
      0.047     58.030
      0.050     64.000
      0.060    152.500
      0.067    210.530
      0.081    305.000
      0.090    363.030
      0.098    420.000
      0.107    427.690
      0.118    422.000
      0.159    363.030
      0.186    305.291
      0.214    233.680
      0.235    300.000
      0.244    316.000
      0.253    321.860
      0.265    317.000
      0.280    300.000
      0.309    267.690
      0.330    292.000
      0.347    297.720
      0.360    292.000
      0.398    276.890
      0.430    290.000
      0.446    293.400
      0.460    290.000
      0.484    280.400
      0.500    285.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)