Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 0.32 mm 
Loading: 
  High-power ion beam
  (in direction <100>)
Experiment type: Laser interferometer (ORVIS) (water window)

     t, ns      V, m/s

      0.000      0.000
      0.652    504.270
      1.902    634.190
      3.311    674.540
      4.603    694.230
      5.873    697.500
      7.102    699.480
      8.462    689.960
      9.823    671.920
     11.704    617.780
     14.120    538.390
     17.466    424.760
     21.367    309.380
     24.811    211.940
     27.400    152.450
     28.684    144.580
     29.941    143.480
     31.315    149.170
     32.634    164.260
     33.939    191.160
     35.245    233.160
     36.800    305.770
     38.035    281.280
     39.458    253.060
     42.103    216.970
     45.581    171.700
     48.962    142.390
     52.211    132.330
     55.404    139.980
     57.709    159.670
     59.458    138.450
     62.825    111.330
     66.331    108.920
     69.739    105.860
     72.662    100.170
     76.098     97.330
     83.193     81.800
     90.579     70.210
     96.889     55.770
    103.714     46.260
    111.440     32.150
    117.840     26.900

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)