Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 3.91 mm 
  Aluminum baseplate 4.7 mm thick
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 660 +/- 20 m/s
  (in direction <111>)
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.090      5.000
      0.110      9.000
      0.127     16.300
      0.140     24.300
      0.173    131.290
      0.260    105.000
      0.280    100.000
      0.303     98.530
      0.310    103.000
      0.330    124.815
      0.370    189.280
      0.380    206.300
      0.427    270.780
      0.461    291.358
      0.510    303.000
      0.562    306.480
      0.602    304.568
      0.665    298.000
      0.725    287.800
      0.798    269.877
      0.880    238.000
      0.934    205.556
      0.995    160.090
      1.032    206.300
      1.078    270.800
      1.100    284.000
      1.122    287.780
      1.150    286.000
      1.180    283.000
      1.265    270.000
      1.427    240.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)