Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 3.7 mm 
  Aluminum baseplate 4.7 mm thick
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 1900 +/- 50 m/s
  (in direction <111>)
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.011     88.980
      0.090    113.470
      0.130    145.000
      0.150    179.780
      0.160    222.470
      0.217    832.470
      0.259    939.259
      0.323   1005.714
      0.417   1030.265
      0.499   1033.651
      0.606    994.000
      0.681    942.280
      0.722    898.330
      0.800    990.000
      0.830   1001.530
      0.860    990.000
      0.915    936.370
      1.000    970.800
      1.070    957.230
      1.200    945.000
      1.400    942.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)