Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 1.34 mm 
  Aluminum baseplate 2 mm thick
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 1250 +/- 50 m/s
  (in direction <111>)
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.010    103.370
      0.027     93.680
      0.042    181.560
      0.048    216.480
      0.056    334.060
      0.061    368.980
      0.069    486.560
      0.077    505.000
      0.086    508.148
      0.101    502.857
      0.119    486.560
      0.169    368.980
      0.182    334.060
      0.207    273.890
      0.227    334.060
      0.247    393.000
      0.251    403.175
      0.258    406.080
      0.269    402.000
      0.279    390.000
      0.306    306.610
      0.338    390.000
      0.346    399.577
      0.349    398.700
      0.356    397.884
      0.364    390.000
      0.387    329.300
      0.420    387.000
      0.427    392.000
      0.433    393.040
      0.437    391.000
      0.444    387.000
      0.470    332.990
      0.511    391.000
      0.517    393.120
      0.540    390.000
      0.600    382.000
      0.831    380.230

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)