Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 0.66 mm 
Loading: 
  High-power ion beam
  (in direction <111>)
Experiment type: Laser interferometer (ORVIS)

     t, ns      V, m/s

      0.000      0.000
      0.812     37.770
      1.569     56.430
      2.367     79.930
      3.422     74.880
      4.887     70.710
      6.262     72.460
      8.129     75.100
     11.427     92.010
     14.564    112.650
     16.578    151.300
     18.126    193.020
     19.715    285.680
     21.340    442.910
     22.291    527.010
     23.013    569.610
     23.700    591.790
     24.387    615.060
     25.075    615.500
     26.255    610.450
     28.920    590.470
     32.183    564.780
     35.481    538.210
     56.230    349.800
     59.493    326.970
     63.165    302.150
     67.004    277.120
     70.517    260.210
     73.585    253.180
     76.758    248.350
     80.000    245.060
     83.672    244.180
     87.934    244.180
     91.343    246.160
     94.564    250.330
     97.813    254.720
    100.930    256.480
    104.547    265.150
    108.656    269.430
    112.058    269.760
    115.341    268.450

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)