Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 0.275 mm (deformed 90-95%)
Loading: 
  Aluminum impactor 0.05 mm thick, impactor velocity 4100 +/- 150 m/s
  (in direction <100>)
Experiment type: Laser interferometer (ORVIS)

     t, ns      V, m/s

      0.000      0.000
      0.847     48.030
      1.958   1594.444
      2.540   1635.185
      3.563   1650.617
      4.533   1643.060
      5.540   1613.580
      7.213   1537.970
      9.261   1419.080
     11.163   1293.290
     11.940   1251.200
     12.558   1226.950
     13.086   1224.100
     13.633   1313.580
     14.215   1380.247
     15.023   1434.770
     15.855   1449.990
     16.293   1443.800
     17.702   1394.350
     19.007   1365.810
     20.278   1354.400
     20.930   1357.250
     21.617   1362.960
     22.339   1385.070
     23.082   1391.250
     24.582   1395.300
     28.726   1393.630
     32.148   1398.390
     35.161   1395.300
     38.272   1395.062
     41.623   1400.617
     45.019   1402.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)