Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 0.1 mm (deformed 90-95%)
Loading: 
  Aluminum impactor 0.05 mm thick, impactor velocity 4100 +/- 150 m/s
  (in direction <100>)
Experiment type: Laser interferometer (ORVIS)

     t, ns      V, m/s

      0.000      0.000
      0.400   2219.577
      0.744   2253.240
      1.010   2237.690
      1.249   2221.830
      1.485   2186.850
      3.682   1791.770
      3.866   1770.400
      4.076   1753.240
      4.256   1765.540
      4.450   1811.850
      4.850   1908.030
      5.050   1956.610
      5.348   1977.660
      5.732   1945.600
      6.338   1886.660
      6.915   1841.320
      7.273   1816.060
      7.581   1810.230
      8.047   1847.150
      8.581   1883.420
      9.063   1888.280
      9.670   1874.350
     10.286   1842.940
     10.837   1822.540
     11.254   1823.510
     11.729   1831.610
     12.313   1847.800
     13.168   1852.660
     19.349   1853.630
     25.547   1853.630

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)