Niobium, R0 =  8.586 g/cc

Target: Niobium single crystal
  Sample density R0 = 8.59 g/cc, bulk sound velocity C0 = 4.44 km/s, longitudial sound velocity Cl = 5.03 km/s
  Sample thickness 0.53 mm 
Loading: 
  High-power ion beam
  (in direction <100>)
Experiment type: Laser interferometer (ORVIS)

     t, ns      V, m/s

      0.000      0.000
      4.119    599.330
      5.150    706.740
      6.181    745.410
      7.212    749.700
      8.243    745.410
     10.305    723.930
     33.502    403.850
     35.049    385.950
     36.080    375.930
     37.380    362.328
     38.657    357.310
     39.508    371.640
     39.801    390.265
     40.425    420.741
     41.342    479.153
     43.297    530.590
     44.328    552.070
     45.359    553.650
     46.390    547.200
     64.432    411.730
     65.979    407.430
     67.010    406.000
     68.041    416.020
     68.635    432.310
     69.552    450.935
     71.134    487.630
     72.165    498.370
     73.196    501.230
     74.742    499.230
     77.320    496.220
     82.475    491.070
     87.630    488.920
     92.785    487.630

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)