Niobium, R0 =  8.586 g/cc

Target: Niobium single crystal
  Sample density R0 = 8.59 g/cc, bulk sound velocity C0 = 4.44 km/s, longitudial sound velocity Cl = 5.03 km/s
  Sample thickness 0.455 mm 
Loading: 
  High-power ion beam
  (in direction <110>)
Experiment type: Laser interferometer (ORVIS)

     t, ns      V, m/s

      0.000      0.000
      1.566    654.109
      2.057    725.000
      2.572    744.330
      3.088    739.500
      3.603    732.250
      4.634    715.330
      5.665    693.580
     18.037    427.750
     19.068    401.170
     20.099    386.670
     20.615    381.830
     21.130    386.670
     21.646    391.500
     22.677    420.500
     23.038    435.000
     23.708    464.000
     24.223    493.000
     24.739    517.170
     25.254    531.670
     26.285    522.000
     34.018    425.330
     35.049    410.830
     36.080    401.170
     36.595    391.500
     37.111    391.500
     37.626    401.170
     38.142    410.830
     39.173    435.000
     39.534    451.920
     40.204    468.830
     40.719    483.330
     41.235    488.170
     41.750    483.330
     42.781    473.670
     43.812    464.000
     46.390    444.670
     48.967    435.000
     51.545    435.000
     54.122    439.830
     56.700    435.000
     59.277    435.000
     64.432    430.170
     69.587    425.330

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)