Niobium, R0 =  8.586 g/cc

Target: Niobium single crystal
  Sample density R0 = 8.59 g/cc, bulk sound velocity C0 = 4.44 km/s, longitudial sound velocity Cl = 5.03 km/s
  Sample thickness 0.49 mm 
Loading: 
  Aluminum impactor 0.05 mm thick, impactor velocity 4100 +/- 150 m/s
  (in direction <100>)
Experiment type: Laser interferometer (ORVIS)

     t, ns      V, m/s

      0.000      0.000
      2.057   1670.640
      2.572   1689.130
      3.088   1679.880
      3.603   1664.470
      7.727   1522.680
     12.882   1325.410
     14.944   1251.440
     15.460   1232.940
     15.975   1226.780
     16.645   1308.460
     17.522   1387.060
     18.037   1417.880
     18.553   1424.050
     19.584   1427.130
     20.615   1417.880
     22.161   1387.060
     24.223   1356.240
     26.285   1325.410
     27.316   1310.000
     27.832   1303.840
     28.347   1300.750
     28.863   1310.000
     29.378   1325.410
     30.409   1356.240
     30.925   1371.650
     31.440   1380.890
     31.956   1383.980
     32.471   1380.890
     33.502   1371.650
     36.080   1340.820
     38.657   1319.250
     40.204   1310.000
     41.235   1306.920
     42.266   1313.080
     43.812   1325.410
     45.359   1331.580
     46.905   1333.120
     47.936   1331.580
     49.483   1325.410
     51.029   1319.250
     52.576   1313.080

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)