Niobium, R0 =  8.586 g/cc

Target: Niobium single crystal
  Sample density R0 = 8.59 g/cc, bulk sound velocity C0 = 4.44 km/s, longitudial sound velocity Cl = 5.03 km/s
  Sample thickness 0.4 mm (deformed 85-90%)
Loading: 
  High-power ion beam
  (in direction <110>)
Experiment type: Laser interferometer (ORVIS)

     t, ns      V, m/s

      0.000      0.000
      0.958     38.040
      1.931    149.850
      2.489    817.730
      3.181    886.700
      4.237    907.420
      5.712    901.860
      9.286    863.510
     12.342    818.350
     15.182    770.720
     16.631    743.000
     18.838    707.470
     21.071    666.190
     22.569    640.000
     25.219    585.460
     28.167    516.340
     32.105    429.120
     35.036    347.940
     35.715    326.130
     35.944    338.977
     37.095    499.640
     38.204    629.070
     39.000    677.000
     40.151    720.460
     41.000    730.000
     41.834    732.990
     42.700    720.000
     43.358    696.340

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)