Niobium, R0 =  8.586 g/cc

Target: Niobium single crystal
  Sample density R0 = 8.59 g/cc, bulk sound velocity C0 = 4.44 km/s, longitudial sound velocity Cl = 5.03 km/s
  Sample thickness 0.09 mm (deformed 85-90%)
Loading: 
  Aluminum impactor 0.05 mm thick, impactor velocity 4100 +/- 150 m/s
  (in direction <110>)
Experiment type: Laser interferometer (ORVIS)

     t, ns      V, m/s

      0.000      0.000
      0.622   2241.623
      0.993   2306.878
      1.819   2352.810
      3.068   2367.190
      4.430   2343.915
      5.783   2264.140
      7.178   2120.760
      7.935   2058.860
      8.303   2041.680
      8.796   2052.070
      9.524   2109.580
     10.559   2195.050
     11.496   2262.950
     12.218   2262.950
     13.086   2219.010
     14.335   2091.210
     15.081   2102.293
     15.640   2110.780
     16.890   2129.950
     18.230   2137.940
     21.298   2122.760
     24.477   2125.950
     31.898   2095.600
     38.882   2076.030

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)