Niobium, R0 =  8.586 g/cc

Target: Niobium single crystal
  Sample density R0 = 8.59 g/cc, bulk sound velocity C0 = 4.44 km/s, longitudial sound velocity Cl = 5.03 km/s
  Sample thickness 0.068 mm (deformed 85-90%)
Loading: 
  Aluminum impactor 0.05 mm thick, impactor velocity 4100 +/- 150 m/s
  (in direction <110>)
Experiment type: Laser interferometer (ORVIS)

     t, ns      V, m/s

      0.000      0.000
      0.777   2504.660
      1.430   2544.640
      1.819   2555.950
      6.366   2584.610
      7.039   2564.250
      7.692   2531.060
      8.310   2483.550
      9.649   2336.860
     10.441   2253.900
     12.593   2034.430
     13.405   2071.760
     14.953   2148.310
     16.682   2167.540
     18.375   2168.670
     20.208   2130.960
     21.444   2060.450
     22.943   1974.090
     24.477   2071.010
     25.817   2125.680
     27.122   2147.560
     29.080   2122.670
     30.961   2062.330
     32.641   2025.000
     34.474   2090.990
     36.626   2133.980
     39.444   2123.420
     41.666   2074.780
     43.554   2030.660
     45.547   2103.440
     47.331   2135.870
     49.392   2125.310
     51.260   2095.890
     52.002   2097.400
     53.273   2104.940

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles