Niobium, R0 =  8.586 g/cc

Target: Niobium single crystal
  Sample density R0 = 8.59 g/cc, bulk sound velocity C0 = 4.44 km/s, longitudial sound velocity Cl = 5.03 km/s
  Sample thickness 0.41 mm (deformed 85-90%)
Loading: 
  High-power ion beam
  (in direction <110>)
Experiment type: Laser interferometer (ORVIS) (water window)

     t, ns      V, m/s

      0.000      0.000
      1.041    896.500
      1.909    898.350
      2.791    887.690
      4.040    852.920
      5.311    815.370
      8.483    731.220
     14.425    577.420
     18.200    490.960
     20.400    447.730
     21.500    418.290
     24.120    369.380
     28.270    287.320
     31.590    225.200
     35.973    146.380
     36.522    137.340
     37.258    141.280
     37.931    156.120
     39.521    277.580
     39.569    279.210
     41.104    408.090
     42.055    461.170
     42.888    485.740
     43.575    488.290
     44.311    486.670
     45.512    471.840
     50.045    408.090
     56.570    319.540
     64.165    220.790
     67.712    170.030
     68.635    155.203
     69.635    148.120
     70.253    152.640
     70.781    171.070
     72.176    214.530
     73.495    249.300
     74.786    269.120
     76.050    283.380
     77.903    294.160
     80.687    292.070
     84.942    262.170
     88.517    231.220
     92.003    201.764
     95.203    174.200
     98.007    152.640

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)