Niobium, R0 =  8.586 g/cc

Target: Niobium single crystal
  Sample density R0 = 8.59 g/cc, bulk sound velocity C0 = 4.44 km/s, longitudial sound velocity Cl = 5.03 km/s
  Sample thickness 3.25 mm 
  Aluminum baseplate 3.9 mm thick
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 700 +/- 20 m/s
  (in direction <100>)
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.078      3.668
      0.120     12.000
      0.135     17.000
      0.154     30.000
      0.160     35.150
      0.200    116.650
      0.215    148.120
      0.250    198.150
      0.267    229.620
      0.295    279.650
      0.320    311.120
      0.355    361.150
      0.400    390.000
      0.420    394.000
      0.454    396.120
      0.500    392.000
      0.625    361.150
      0.750    311.120
      0.810    279.650
      0.867    229.620
      0.889    203.870
      0.911    229.620
      0.940    279.650
      0.960    311.120
      0.990    338.000
      1.020    340.850
      1.058    338.765
      1.100    334.000
      1.215    311.120
      1.302    297.210
      1.380    315.000
      1.411    318.100
      1.450    315.000
      1.498    309.530
      1.998    309.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)