Niobium, R0 =  8.586 g/cc

Target: Niobium single crystal
  Sample density R0 = 8.59 g/cc, bulk sound velocity C0 = 4.44 km/s, longitudial sound velocity Cl = 5.03 km/s
  Sample thickness 1.36 mm 
  Aluminum baseplate 0.77 mm thick
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 1250 +/- 40 m/s
  (in direction <110>)
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.020      5.000
      0.030      8.000
      0.037     15.000
      0.039     28.000
      0.042     48.940
      0.045    152.500
      0.063    610.000
      0.067    678.000
      0.071    693.898
      0.075    698.413
      0.082    701.000
      0.085    698.413
      0.091    696.155
      0.110    658.940
      0.129    609.806
      0.154    506.440
      0.162    457.500
      0.178    305.700
      0.224    506.440
      0.235    560.000
      0.245    578.000
      0.255    582.690
      0.342    560.705
      0.392    556.160
      0.460    550.150

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)