Nickel, R0 =  8.875 g/cc

Target: 
  Sample density R0 = 8.86 g/cc, bulk sound velocity C0 = 4.57 km/s, longitudial sound velocity Cl = 5.63 km/s
  Sample thickness 0.4 mm (sheet)
Loading: 
  High-power ion beam
Experiment type: Laser interferometer (ORVIS) (water window)

     t, ns      V, m/s

      0.000      0.000
      1.798     21.600
      2.784     36.210
      3.894     73.700
      4.198    794.356
      4.797    805.996
      5.998    812.470
      7.178    805.480
      8.483    792.780
     10.335    765.079
     13.752    712.940
     28.073    459.450
     31.211    406.080
     33.259    379.820
     33.912    368.590
     34.557    367.320
     35.231    367.960
     36.591    380.240
     37.751    398.030
     39.812    414.130
     42.075    426.410
     43.957    425.770
     45.422    421.960
     47.539    410.310
     49.476    401.210
     52.072    382.570
     54.030    373.680
     56.022    366.050
     57.730    360.120
     59.826    357.370
     61.999    355.680
     64.450    356.520
     66.990    358.430
     69.031    357.580
     70.940    351.860
     72.808    349.530
     74.814    346.360
     76.772    339.370
     79.347    330.260
     82.644    321.580
     86.719    311.410
     90.371    303.790
     93.772    300.190
     97.001    297.650

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)