Tin, R0 =  7.300 g/cc

Target: 
  Sample density R0 = 7.29 g/cc, bulk sound velocity C0 = 2.61 km/s, longitudial sound velocity Cl = 3.43 km/s
  Sample thickness 4 mm (cast and pressed)
  Aluminum baseplate 4 mm thick
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.042      2.330
      0.084    459.230
      0.090    474.921
      0.106    499.630
      0.119    512.110
      0.148    540.030
      0.172    552.510
      0.195    562.540
      0.230    567.619
      0.271    564.233
      0.310    552.510
      0.359    540.030
      0.431    512.110
      0.485    489.030
      0.540    512.110
      0.586    527.407
      0.620    532.000
      0.749    515.910
      0.865    522.920
      0.992    518.920
      1.098    521.480
      1.277    518.900
      1.404    518.620
      1.921    518.540

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)