Titanium, R0 =  4.527 g/cc

Target: Titanum of high purity
  Sample density R0 = 4.5 g/cc, bulk sound velocity C0 = 5.12 km/s, longitudial sound velocity Cl = 6.15 km/s
  Sample thickness 2.06 mm 
  Aluminum baseplate 0.78 mm thick
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 660 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.057     18.350
      0.070     26.000
      0.083     40.010
      0.089     99.850
      0.090    121.510
      0.097    181.350
      0.101    203.010
      0.112    262.850
      0.120    284.510
      0.141    344.350
      0.159    366.010
      0.174    372.628
      0.189    373.730
      0.200    370.000
      0.216    343.422
      0.242    284.510
      0.249    262.850
      0.270    203.010
      0.277    181.350
      0.307    121.510
      0.330     99.850
      0.350     86.000
      0.370     81.975
      0.390     88.000
      0.430    110.000
      0.446    112.290
      0.470    110.000
      0.497     99.850
      0.540     81.000
      0.580     68.000
      0.620     63.000
      0.670     58.750

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)