Titanium, R0 =  4.527 g/cc

Target: Titanum of high purity
  Sample density R0 = 4.5 g/cc, bulk sound velocity C0 = 5.12 km/s, longitudial sound velocity Cl = 6.15 km/s
  Sample thickness 2.29 mm 
  Aluminum baseplate 0.77 mm thick
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 1250 +/- 40 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.030     10.000
      0.040     20.000
      0.053     40.000
      0.059     78.360
      0.062    427.770
      0.093    840.860
      0.096    885.270
      0.105    930.000
      0.115    948.000
      0.118    952.290
      0.130    946.000
      0.140    930.000
      0.161    885.270
      0.175    840.860
      0.203    732.770
      0.225    643.220
      0.240    732.770
      0.260    805.000
      0.266    820.000
      0.276    833.620
      0.290    830.000
      0.300    820.000
      0.340    760.000
      0.353    747.670
      0.380    776.000
      0.392    781.290
      0.410    775.000
      0.460    755.000
      0.490    745.790
      0.510    750.000
      0.550    765.000
      0.566    770.350
      0.613    753.030

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)