Titanium, R0 =  4.527 g/cc

Target: Titanum of high purity
  Sample density R0 = 4.5 g/cc, bulk sound velocity C0 = 5.12 km/s, longitudial sound velocity Cl = 6.15 km/s
  Sample thickness 4.4 mm 
  Aluminum baseplate 2 mm thick
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 660 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.150     19.000
      0.180     24.000
      0.200     31.000
      0.211     41.760
      0.213    101.120
      0.224    123.260
      0.234    204.120
      0.245    264.760
      0.255    286.260
      0.288    427.120
      0.310    469.260
      0.360    530.760
      0.390    560.000
      0.424    565.940
      0.470    564.000
      0.525    560.000
      0.565    555.000
      0.661    530.760
      0.715    505.620
      0.785    449.260
      0.805    427.120
      0.862    367.760
      0.880    345.620
      0.923    306.600
      0.964    345.620
      0.986    367.760
      1.050    430.000
      1.080    450.000
      1.100    460.000
      1.130    470.000
      1.185    475.000
      1.250    470.000
      1.305    460.000
      1.343    450.000
      1.407    427.120
      1.435    409.000
      1.460    401.460
      1.480    404.000
      1.541    427.120
      1.570    437.000
      1.630    451.000
      1.681    457.000
      1.721    460.000
      1.782    462.470
      1.832    460.000
      1.857    457.000
      1.888    451.000
      1.947    432.000
      1.995    416.000
      2.043    410.310
      2.080    417.000
      2.110    425.000
      2.184    437.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)