Titanium, R0 =  4.527 g/cc

Target: Titanum of high purity
  Sample density R0 = 4.5 g/cc, bulk sound velocity C0 = 5.12 km/s, longitudial sound velocity Cl = 6.15 km/s
  Sample thickness 4.3 mm 
  Aluminum baseplate 2 mm thick
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 1900 +/- 70 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.035     10.000
      0.050     35.000
      0.060     40.000
      0.069     71.390
      0.075    354.700
      0.081    472.381
      0.086    528.890
      0.096    681.390
      0.103    812.200
      0.108    964.700
      0.117   1138.890
      0.138   1291.390
      0.170   1400.000
      0.220   1470.000
      0.280   1494.680
      0.340   1480.000
      0.400   1440.000
      0.550   1291.390
      0.610   1238.890
      0.664   1189.310
      0.690   1238.890
      0.720   1291.390
      0.770   1370.000
      0.790   1390.000
      0.812   1401.460
      0.840   1401.000
      0.855   1396.000
      0.870   1390.000
      0.900   1380.000
      1.000   1300.000
      1.161   1179.000
      1.300   1229.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)