Titanium, R0 =  4.527 g/cc

Target: Titanum of high purity
  Sample density R0 = 4.5 g/cc, bulk sound velocity C0 = 5.12 km/s, longitudial sound velocity Cl = 6.15 km/s
  Sample thickness 0.78 mm 
Loading: 
  High-power ion beam
Experiment type: Laser interferometer (ORVIS)

     t, ns      V, m/s

      0.000      0.000
      0.768      2.420
      1.799     33.830
      2.572     48.330
      4.119     67.670
      5.150     91.830
      6.181    140.170
      6.696    188.500
      8.243    319.000
      9.274    415.670
      9.789    449.500
     10.820    464.000
     11.903    483.330
     12.831    512.330
     13.398    536.500
     14.944    657.330
     15.975    729.830
     16.903    778.170
     18.037    816.830
     19.068    826.500
     20.099    816.830
     21.130    802.330
     52.060    367.330
     57.215    319.000
     62.370    290.000
     64.948    285.170
     66.494    290.000
     67.525    294.830
     68.556    319.000
     69.587    343.170
     70.618    391.500
     71.649    439.830
     72.680    464.000
     74.227    488.170
     76.289    497.830
     77.835    493.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)