Sapphire, R0 =  3.977 g/cc

Target: Al2O3 (ruby)
  Sample density R0 = 3.99 g/cc, longitudial sound velocity Cl = 11.2 km/s
  Sample thickness 4.98 mm 
  Aluminum baseplate 2 mm thick
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 660 +/- 20 m/s
  (perpendicular to {1100})
Experiment type: Laser interferometer (VISAR) (water window)

     t, mks     V, m/s

      0.000      0.000
      0.010      5.000
      0.019     20.000
      0.024    171.300
      0.031    224.339
      0.045    265.000
      0.050    270.000
      0.060    277.500
      0.070    270.000
      0.107    223.386
      0.140    171.300
      0.200     71.620
      0.250     28.610
      0.290     19.000
      0.350     21.690
      0.420     18.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)