Sapphire, R0 =  3.977 g/cc

Target: Al2O3 (ruby)
  Sample density R0 = 3.99 g/cc, longitudial sound velocity Cl = 11.2 km/s
  Sample thickness 3.63 mm 
  Aluminum baseplate 1.98 mm thick
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 660 +/- 20 m/s
  (perpendicular to {1120})
Experiment type: Laser interferometer (VISAR) (water window)

     t, mks     V, m/s

      0.000      0.000
      0.039      4.310
      0.055     20.000
      0.060    186.050
      0.070    235.000
      0.090    278.200
      0.150    235.290
      0.200    186.050
      0.280     82.790
      0.322     39.550
      0.350     20.000
      0.385      7.500
      0.417      4.220
      0.443     12.530
      0.478      5.750
      0.525     10.740

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)