Sapphire, R0 =  3.977 g/cc

Target: Al2O3 (ruby)
  Sample density R0 = 3.99 g/cc, longitudial sound velocity Cl = 11.2 km/s
  Sample thickness 2.22 mm 
  Aluminum baseplate 4 mm thick
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 1250 +/- 50 m/s
  (perpendicular to {1120})
Experiment type: Laser interferometer (VISAR) (water window)

     t, mks     V, m/s

      0.000      0.000
      0.020     25.230
      0.035     77.130
      0.040    229.630
      0.042    482.730
      0.045    508.148
      0.052    524.540
      0.060    520.423
      0.083    482.730
      0.125    382.130
      0.146    330.230
      0.183    229.630
      0.206    182.434
      0.246    128.880
      0.259    229.630
      0.272    318.270

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)