Sapphire, R0 =  3.977 g/cc

Target: Al2O3 (ruby)
  Sample density R0 = 3.99 g/cc, longitudial sound velocity Cl = 11.2 km/s
  Sample thickness 3.65 mm 
  Aluminum baseplate 2 mm thick
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 1250 +/- 50 m/s
  (perpendicular to {1120})
Experiment type: Laser interferometer (VISAR) (water window)

     t, mks     V, m/s

      0.000      0.000
      0.010      4.000
      0.020      9.960
      0.020    620.250
      0.060    564.990
      0.080    526.170
      0.100    477.000
      0.120    412.490
      0.130    370.123
      0.150    259.990
      0.160    180.520
      0.170    550.000
      0.170    564.990
      0.200    526.170
      0.230    480.000
      0.260    412.490
      0.272    374.321
      0.300    259.990

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)