Steel 35h3NM, R0 =  7.760 g/cc

Target: 
  Sample density R0 = 7.76 g/cc, bulk sound velocity C0 = 4.65 km/s, longitudial sound velocity Cl = 5.89 km/s
  Sample thickness 11.5 mm (rod, batch II)
Loading: 
  High explosive in contact with sample
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.030     61.000
      0.050    102.000
      0.210    261.000
      0.250    282.000
      0.280    316.000
      0.290    337.000
      0.320    371.000
      0.330    392.000
      0.340    426.000
      0.370    447.000
      0.750    452.000
      1.280    447.000
      1.850    426.000
      2.430    398.000
      2.930    371.000
      3.510    337.000
      3.820    321.000
      3.900    337.000
      4.200    392.000
      4.530    426.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)