Aluminum AD1, R0 =  2.710 g/cc

Target: 
  Sample density R0 = 2.71 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 10 mm (rod)
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 4000 +/- 150 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.050      8.000
      0.248     16.000
      0.252    150.000
      0.252    199.000
      0.262   3901.000
      0.262   3934.000
      0.262   4025.000
      0.274   4028.000
      0.334   3984.000
      0.392   3951.000
      0.477   3916.000
      0.536   3924.000
      0.601   3915.000
      0.693   3893.000
      0.821   3898.000
      0.973   3881.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)