Aluminum AMg6M, R0 =  2.610 g/cc

Target: 
  Sample density R0 = 2.61 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 9.6 mm (sheet)
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 660 +/- 20 m/s
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.050     40.000
      0.200     72.000
      0.230    100.000
      0.250    168.000
      0.282    261.905
      0.300    283.000
      0.370    250.000
      0.452    187.513
      0.470    170.000
      0.536    191.005
      0.570    197.000
      0.620    185.000
      0.670    167.000
      0.750    181.000
      0.840    166.000
      0.920    172.000
      1.350    171.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)