Aluminum AMg6M, R0 =  2.610 g/cc

Target: 
  Sample density R0 = 2.61 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 4.5 mm (sheet)
  Copper baseplate 4 mm thick
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 5300 +/- 150 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.040      0.000
      0.050      7.000
      0.055     20.000
      0.057    110.000
      0.057    199.000
      0.062   4701.000
      0.062   4780.000
      0.063   4870.000
      0.063   4887.000
      0.067   4890.000
      0.075   4885.000
      0.170   4757.000
      0.200   4790.000
      0.210   4800.000
      0.230   4804.000
      0.245   4800.000
      0.280   4786.000
      0.320   4787.000
      0.340   4788.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)