Iron , R0 =  7.800 g/cc

Target: 
  Sample density R0 = 7.8 g/cc, bulk sound velocity C0 = 4.65 km/s, longitudial sound velocity Cl = 5.97 km/s
  Sample thickness 20 mm (rod)
Loading: 
  High explosive in contact with sample
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.100     38.000
      0.300     39.000
      0.500     52.000
      0.600     64.000
      0.700    110.000
      0.730    200.000
      0.834    417.813
      0.900    467.000
      1.000    474.000
      1.100    476.000
      1.500    460.000
      2.000    429.000
      2.460    404.000
      2.700    422.000
      3.000    433.000
      3.300    429.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)