Iron , R0 =  7.800 g/cc

Target: 
  Sample density R0 = 7.8 g/cc, bulk sound velocity C0 = 4.65 km/s, longitudial sound velocity Cl = 5.97 km/s
  Sample thickness 10 mm (rod)
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 590 +/- 20 m/s
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.060     45.000
      0.100     39.000
      0.200     39.000
      0.300     48.000
      0.400     93.000
      0.520    300.000
      0.545    315.485
      0.580    319.000
      0.626    316.614
      0.700    308.000
      0.800    285.000
      0.900    256.000
      0.970    239.000
      1.065    267.513
      1.120    275.000
      1.340    255.000
      1.550    263.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)